timschneider 1ac3b466da Meltingplot PLA: raise slow_down_layer_time by calibration factor 1.5
Print feedback on CHX 350 with a 0.8 nozzle at 0.44 mm layer height showed
curling at the retraction points with the derived value of 25 s. There is no
cooling headroom left to trade: fdm_filament_pla pins fan_min_speed =
fan_max_speed = 100, and additional_cooling_fan_speed is inert because no
Meltingplot machine enables auxiliary_fan. Minimum layer time is the only
remaining lever; 35 s prints cleanly at that geometry.

The cross-section rule only fixes the ratios between nozzle sizes, so this
is a calibration of the PLA anchor itself: both PLA ladders are scaled by
1.5 (Extrudr 9/20/38/56/83 s, Meltingplot PLA 8/17/30/45/66 s for
0.4/0.6/0.8/1.0/1.2). The Extrudr base fan_cooling_layer_time goes 60 -> 100
so the 1.2-nozzle value stays below it.

Other materials are left unchanged - only the PLA anchor has a real
counter-example so far.